TITAN
®
% Density* Energy Recomm Recomm Water
Emulsion ANFO (g/cm
3
) (MJ/kg) sleep time minimum hole Resistance
Product (wt%) (days) diameter (mm)
TITAN2000G(Gassed) 0 1.05-1.25* 2.5 12 102 Excellent
TITAN2010(HeavyANFO) 90 0.86
#
3.6 14
ø
102 Poor
TITAN2020(HeavyANFO) 80 0.97
#
3.4 14
ø
102 Poor
TITAN2030(HeavyANFO) 70 1.10
#
3.3 14
ø
102 Poor
TITAN2040(HeavyANFO) 60 1.25
#
3.2 14
ø
127 Poor
TITAN2050(Blend) 50 1.32
#
3.1 14 203 Average
TITAN2050G(Gassed) 50 1.20-1.25* 3.1 12 102 Average
TITAN2060G(Gassed) 40 1.05-1.25* 3.0 12 102 Good
TITAN2070G(Gassed) 30 1.05-1.25* 2.9 12 102 Excellent
TITAN2080G(Gassed) 20 1.05-1.25* 2.7 12 102 Excellent
TITAN2090G(Gassed) 10 1.05-1.25* 2.6 12 102 Excellent
TITAN3000G(Gassed) 0 1.05-1.25* 2.7 12 76 Excellent
TITAN3010(HeavyANFO) 90 0.86
#
3.6 14
ø
89 Poor
TITAN3020(HeavyANFO) 80 0.93
#
3.5 14
ø
89 Poor
TITAN3030(HeavyANFO) 70 1.05
#
3.4 14
ø
102 Poor
TITAN3040(HeavyANFO) 60 1.23
#
3.3 14
ø
127 Poor
TITAN3060G(Gassed) 40 1.05-1.25* 3.1 12 89 Good
TITAN3070G(Gassed) 30 1.05-1.25* 3.0 12 76 Excellent
TITAN3080G(Gassed) 20 1.05-1.25* 2.9 12 76 Excellent
TITAN3090G(Gassed) 10 1.05-1.25* 2.8 12 76 Excellent
TITAN4000G(Gassed) 0 1.05-1.25* 2.4 12 102 Excellent
TITAN4010(HeavyANFO) 90 0.85
#
3.6 12
ø
102 Poor
TITAN4020(HeavyANFO) 80 0.96
#
3.4 12
ø
102 Poor
TITAN4030(HeavyANFO) 70 1.10
#
3.3 12
ø
102 Poor
TITAN4040(HeavyANFO) 60 1.26
#
3.2 12
ø
152 Poor
TITAN4050(Blend) 50 1.32
#
3.0 12 152 Average
TITAN4050G(Gassed) 50 1.05-1.25* 3.0 12 102 Average
TITAN4060G(Gassed) 40 1.05-1.25* 2.9 12 102 Good
TITAN4070G(Gassed) 30 1.05-1.25* 2.8 12 102 Excellent
TITAN4080G(Gassed) 20 1.05-1.25* 2.6 12 102 Excellent
TITAN4090G(Gassed) 10 1.05-1.25* 2.5 12 102 Excellent
TITAN5000G(Gassed) 0 1.05-1.25* 2.7
^
102 Excellent
TITAN5010(HeavyANFO) 90 0.88
#
3.6
^
102 Poor
TITAN5020(HeavyANFO) 80 0.94
#
3.5
^
102 Poor
TITAN5030(HeavyANFO) 70 1.05
#
3.4
^
102 Poor
TITAN5040(HeavyANFO) 60 1.21
#
3.3
^
152 Poor
TITAN5050(HeavyANFO) 50 1.31
#
3.2
^
203 Average
TITAN5060(Blend) 40 1.32
#
3.0
^
250 Good
TITAN5060G(Gassed) 40 1.05-1.25* 3.1
^
102 Good
TITAN5065G(Gassed) 35 1.05-1.25* 3.0
^
102 Good
TITAN5070G(Gassed) 30 1.05-1.25* 3.0
^
102 Excellent
TITAN5080G(Gassed) 20 1.05-1.25* 2.9
^
102 Excellent
TITAN5090G(Gassed) 10 1.05-1.25* 2.8
^
102 Excellent
TITAN7000(Gassed) 0 0.80-1.25 2.9 30
†
35 Excellent
TITAN7000i(Gassed) 0 0.80-1.25 2.9
^
35 Excellent
TITAN7000SX(Gassed) 0 0.80-1.25 2.8
^
35 Excellent
* Inholegassedproductdensityisdependentonholedepth.
#
DensitiesmayvaryduetovariationsintheANprilldensity.Forblendswith50%emulsionorgreater,pleaseconsultyour
DynoNobelrepresentativetoensuretheproductissuitableforyourapplication.
ø
Forunreactivegroundindryholeconditionswithnowaterpresent.Dewateredholesmayreducesleeptime.
^
ForapplicationsinreactivegroundconditionspleaseconsultyourDynoNobelrepresentativetoundertaketheappropriate
testworkpriortothedevelopmentofsuitablesitespecificprocedures.
†
Forupholeapplications,sleeptimesaredependentongeology,waterandinholeconditions.
Bulk products